Special grade | C | Si | Mn | Cr |
TG4241 | 0.90-0.95 | 0.80-1.20 | 0.25-0.40 | 4.00-4.50 |
TG4341 | 0.83-0.93 | 0.70-1.00 | 0.20-0.40 | 3.80-4.50 |
Mo | V | W | P | S |
1.00-1.20 | 0.80-1.00 | 1.80-2.50 | ≤0.030 | ≤0.020 |
2.50-3.50 | 1.20-1.80 | 3.50-4.50 | ≤0.030 | ≤0.020 |
Under Annealed Condition : |
Reduction Ratio : |
Delivery Status : |
Hardness : HB205-255 |
As 1:4 or 1:5 |
As Cold drawn / Hot rolled / forged, in annealed condition |
Sizes of Round Bars :
Cold Drawn/Ground Bar |
Hot Rolled Annealed Peeled Bar |
Forged Anealed Turned Bar |
Coil |
Φ 2.0 - 14.4mm |
Φ 14.5 - 80.0mm |
Φ 81.0 - 255.0mm |
Φ 2.0 - 13.5mm |
Sizes of Flat Bars :
Thickness |
Width |
5mm - 150mm |
5mm - 810mm |
Sizes of Square Bars :
4mm - 100mm |
Sizes of Sheets :
Thickness |
Width |
Length |
0.5mm - 12mm |
810mm |
2500mm |
Heat Treatments :
Annealing temperature : 860-880℃, keep this temperature by 2-4 hours, then cooling to 600℃ in the speed of less than 30℃/h.
If after cold drawn process, suggest and stress relieving annealing process. Under the temperature of 600-700℃, keep this temperature by 2 hours.
Quenching & Tempering (salt bath).
Heating temperature under: 400-500℃ and 850-900℃
TG4241 Austenitizing temperature: 1150-1180℃
TG4341 Austenitizing temperature: 1160-1190℃
Heating coefficient 10-15sec/mm, quenching under 580-620℃, then cooling to room temperature.
Quenching temperature difference in 5-10℃ between TGM2, TGM2A;
TGM2A's quenching temperature is higher than TGM2
Tempering temperature under:540-560℃, tempering 3 times, each time 1 hour, then cooling to room temperature.